ASME SA240
Glomet Stainless supplies hot rolled annealed and pickled plates (No.1 finish) and cold rolled plates in stainless steel, duplex, titanium and nickel alloys. Plates are supplied to ASTM A240 / ASME SA240, and to ASTM B265 or the matching ASTM B specification for titanium and nickel grades.
Take full mill plates, or let us plasma, waterjet or gas cut blanks, circles, rings and flange blanks to your drawing. Pressure vessel plates are supplied with heat-traceable mill test certificates, and ultrasonic testing can be arranged on request.
Dual-certified 304/304L and 316/316L plates cover most vessel and tank work; 321, 347 and 310S for elevated temperature.
304/304L316/316L321347310SHigher strength lets designers reduce wall thickness on vessels, while improving chloride pitting resistance.
S31803S32205S32750S32760Used for tube sheets, seawater and chlor-alkali equipment where stainless steels pit or crack.
Gr 1Gr 2Gr 5Gr 7Gr 12For furnaces, acid service, flue gas desulphurisation and marine equipment.
Inconel 600/625Incoloy 800/825Monel 400C276Ni 200| Grade | C | Mn | Si | P | S | Cr | Ni | Mo | N | Other |
|---|---|---|---|---|---|---|---|---|---|---|
| 304 | 0.08 | 2.00 | 0.75 | 0.045 | 0.030 | 18.0–20.0 | 8.0–10.5 | – | 0.10 | – |
| 304L | 0.030 | 2.00 | 0.75 | 0.045 | 0.030 | 17.5–19.5 | 8.0–12.0 | – | 0.10 | – |
| 316 | 0.08 | 2.00 | 0.75 | 0.045 | 0.030 | 16.0–18.0 | 10.0–14.0 | 2.00–3.00 | 0.10 | – |
| 316L | 0.030 | 2.00 | 0.75 | 0.045 | 0.030 | 16.0–18.0 | 10.0–14.0 | 2.00–3.00 | 0.10 | – |
| 321 | 0.08 | 2.00 | 0.75 | 0.045 | 0.030 | 17.0–19.0 | 9.0–12.0 | – | 0.10 | Ti 5×(C+N) – 0.70 |
| 310S | 0.08 | 2.00 | 1.50 | 0.045 | 0.030 | 24.0–26.0 | 19.0–22.0 | – | – | – |
| 904L | 0.020 | 2.00 | 1.00 | 0.045 | 0.035 | 19.0–23.0 | 23.0–28.0 | 4.0–5.0 | 0.10 | Cu 1.0–2.0 |
| Duplex 2205 (S32205) | 0.030 | 2.00 | 1.00 | 0.030 | 0.020 | 22.0–23.0 | 4.5–6.5 | 3.0–3.5 | 0.14–0.20 | – |
| Super Duplex 2507 (S32750) | 0.030 | 1.20 | 0.80 | 0.035 | 0.020 | 24.0–26.0 | 6.0–8.0 | 3.0–5.0 | 0.24–0.32 | Cu 0.50 |
| Grade | Ni | Cr | Mo | Fe | Cu | C | Mn | Si | Other |
|---|---|---|---|---|---|---|---|---|---|
| Titanium Gr 2 | – | – | – | 0.30 | – | 0.08 | – | – | O 0.25, N 0.03, H 0.015, Ti bal. |
| Titanium Gr 5 | – | – | – | 0.40 | – | 0.08 | – | – | Al 5.5–6.75, V 3.5–4.5, O 0.20, Ti bal. |
| Inconel 600 | 72.0 min | 14.0–17.0 | – | 6.0–10.0 | 0.50 | 0.15 | 1.00 | 0.50 | S 0.015 |
| Inconel 625 | 58.0 min | 20.0–23.0 | 8.0–10.0 | 5.0 | – | 0.10 | 0.50 | 0.50 | Nb+Ta 3.15–4.15 |
| Incoloy 800 | 30.0–35.0 | 19.0–23.0 | – | 39.5 min | 0.75 | 0.10 | 1.50 | 1.00 | Al 0.15–0.60, Ti 0.15–0.60 |
| Incoloy 825 | 38.0–46.0 | 19.5–23.5 | 2.5–3.5 | 22.0 min | 1.5–3.0 | 0.05 | 1.00 | 0.50 | Ti 0.6–1.2 |
| Monel 400 | 63.0 min | – | – | 2.50 | 28.0–34.0 | 0.30 | 2.00 | 0.50 | S 0.024 |
| Hastelloy C276 | Balance | 14.5–16.5 | 15.0–17.0 | 4.0–7.0 | – | 0.010 | 1.00 | 0.08 | W 3.0–4.5, Co 2.5 |
| Nickel 200 | 99.0 min | – | – | 0.40 | 0.25 | 0.15 | 0.35 | 0.35 | S 0.01 |
Weight %, maximum unless a range is shown. The mill test certificate supplied with each heat is the controlling document.
| Grade | Tensile Strength (MPa, min) | Yield Strength 0.2% (MPa, min) | Elongation (% in 50 mm, min) | Hardness (max) |
|---|---|---|---|---|
| 304 | 515 | 205 | 40 | 201 HBW / 92 HRB |
| 304L | 485 | 170 | 40 | 201 HBW / 92 HRB |
| 316 | 515 | 205 | 40 | 217 HBW / 95 HRB |
| 316L | 485 | 170 | 40 | 217 HBW / 95 HRB |
| 321 | 515 | 205 | 40 | 217 HBW / 95 HRB |
| 310S | 515 | 205 | 40 | 217 HBW / 95 HRB |
| 904L | 490 | 220 | 35 | 90 HRB |
| Duplex 2205 (S32205) | 655 | 450 | 25 | 293 HBW / 31 HRC |
| Super Duplex 2507 (S32750) | 795 | 550 | 15 | 310 HBW / 32 HRC |
| Grade | Tensile Strength (MPa, min) | Yield Strength 0.2% (MPa, min) | Elongation (%, min) | Condition |
|---|---|---|---|---|
| Titanium Gr 2 | 345 | 275 | 20 | Annealed |
| Titanium Gr 5 | 895 | 828 | 10 | Annealed |
| Inconel 600 | 550 | 240 | 30 | Annealed |
| Inconel 625 | 827 | 414 | 30 | Annealed (Grade 1) |
| Incoloy 800 | 520 | 205 | 30 | Annealed |
| Incoloy 825 | 586 | 241 | 30 | Annealed |
| Monel 400 | 483 | 193 | 35 | Annealed |
| Hastelloy C276 | 690 | 283 | 40 | Solution Annealed |
| Nickel 200 | 380 | 103 | 40 | Annealed |
Room temperature values for annealed plate. Limits can vary with thickness — confirm against the ordered specification.





Share the grade, thickness, plate size or cutting drawing and quantity. We quote with stock availability and delivery time.